Manmade TextilesTextile Fibres

Manufacturing of Acrylic Fibres by Solution Spinning

The most commonly used fibre-spinning methods for acrylic and modacrylic fibres are wet spinning and dry spinning. These polymers cannot normally be melt-spun because they degrade before reaching a suitable melting condition. The selection of spinning method depends on polymer composition, solvent, spinning-dope properties and the required fibre characteristics.

1. Wet Spinning of Acrylic Fibres

Wet spinning is a solution-spinning method in which polymer solution is extruded into a coagulation bath containing a non-solvent. The solvent diffuses out of the extruded polymer solution, while the non-solvent enters the filament. This causes the polymer to coagulate and form a solid filament.

1.1 Process Flowchart

Polymer preparation
↓
Dissolution in suitable solvent
↓
Spinning dope preparation
↓
Filtration and deaeration
↓
Extrusion through spinneret
↓
Coagulation in spinning bath
↓
Washing
↓
Drawing or stretching
↓
Drying
↓
Crimping
↓
Annealing and finishing
↓
Cutting and packaging

1.2 Step-by-Step Process

Step 1: Preparation of Spinning Dope

The acrylic polymer is dissolved in a suitable solvent to prepare a viscous spinning solution called dope.

Common organic solvents include:

  • Dimethylformamide (DMF)
  • Dimethylacetamide (DMAc)
  • Dimethyl sulphoxide (DMSO)

Other solvent systems include concentrated aqueous solutions of:

  • Sodium thiocyanate
  • Zinc chloride
  • Nitric acid

The choice of solvent depends on polymer composition and molecular weight. The polymer concentration must be controlled to obtain suitable dope viscosity and spinning behaviour.

Step 2: Filtration and Deaeration

The spinning dope is prepared carefully to obtain a uniform solution. Undissolved polymer particles and other impurities must be removed before spinning. Air bubbles are also removed to improve spinning performance.

Step 3: Extrusion Through Spinneret

The spinning dope is supplied to the spinneret using a metering system.

The spinneret contains many small holes. The polymer solution passes through these holes and forms continuous liquid filaments.

Step 4: Coagulation

The extruded filaments enter a coagulation bath containing a non-solvent. During coagulation:

  • Solvent moves out of the filament.
  • Non-solvent moves into the filament.
  • The polymer separates from the solution.
  • The liquid filament becomes a gel-like solid filament.

This process is called coagulation. The coagulation conditions influence the internal structure and cross-section of the resulting fibres.

Step 5: Washing

The coagulated filaments are washed to remove residual solvent. Hot water is commonly used for washing in the described acrylic fibre process.

Step 6: Drawing or Stretching

The filaments are stretched to improve molecular orientation and fibre properties. Drawing can take place during subsequent processing, including washing and drying. The degree of stretching influences the mechanical behaviour of the resulting fibre.

Step 7: Drying

After washing and finish application, the tow still contains water and must be dried. Drying can be carried out using:

  • Heated drums or calenders
  • Hot air
  • Other suitable heating arrangements

Acrylic tow is generally dried at 120–170°C in the described process. Drying conditions influence shrinkage and setting behaviour.

Step 8: Crimping

Crimping introduces a wavy or zigzag structure into the fibres.

It improves:

  • Fibre-to-fibre cohesion
  • Spinnability
  • Handling during subsequent textile processing

Crimping is an important operation in acrylic staple-fibre production.

Step 9: Annealing and Finishing

Annealing is used to relieve internal stresses developed during drawing and processing. Finishing provides the required surface characteristics for further handling and processing.

Step 10: Cutting and Packaging

The processed tow is cut into staple fibres of the required length and then packed for further textile processing.

2. Dry Spinning of Acrylic Fibres

Dry spinning is a solution-spinning process in which the polymer solution is extruded through a spinneret into a heated chamber. The solvent evaporates from the extruded filaments, leaving solid polymer filaments.

2.1 Process Flowchart

Polymer preparation
↓
Dissolution in volatile organic solvent
↓
Spinning dope preparation
↓
Filtration and deaeration
↓
Extrusion through spinneret
↓
Passage through heated spinning chamber
↓
Solvent evaporation and recovery
↓
Solid filament formation
↓
Finish application
↓
Winding or tow formation
↓
Drawing and post-spinning processing

2.2 Step-by-Step Process

Step 1: Preparation of Spinning Dope

The acrylic polymer is dissolved in a suitable organic solvent. DMF is an important solvent used for dry spinning. The dope must have suitable polymer concentration and viscosity for stable extrusion.

Step 2: Filtration and Deaeration

The dope is filtered to remove impurities and undissolved particles. Air bubbles are removed to ensure uniform filament formation.

Step 3: Extrusion Through Spinneret

The polymer solution is extruded through the spinneret holes to form liquid filaments.

Step 4: Solvent Evaporation

The filaments pass through a heated spinning chamber. Hot gas is used to evaporate the solvent from the filaments.

As the solvent evaporates, the polymer concentration increases and the filaments solidify.

Step 5: Solvent Recovery

The solvent vapour is collected and recovered. Solvent recovery is important in dry spinning because a considerable amount of solvent is used in the spinning dope.

Step 6: Finish Application

A suitable finish is applied to the filaments as they leave the spinning chamber.

Step 7: Tow Formation and Winding

Filaments from several spinning positions are combined to form a tow.

The tow is collected in suitable containers for further processing.

Step 8: Further Processing

The tow is subjected to drawing, drying, crimping, annealing and cutting as required.

3. Difference Between Wet and Dry Spinning of Acrylic Fibres

FeatureWet spinningDry spinning
PrincipleCoagulation in a non-solvent bathSolvent evaporation in a heated chamber
Spinning mediumCoagulation bathHeated gas or air
Filament solidificationSolvent and non-solvent exchangeSolvent evaporation
Solvent removalWashingEvaporation and recovery
Fibre structureCan contain internal voidsGenerally more regular and compact
Cross-sectionCan be bean-shaped or circularOften dog-bone shaped
Fine-denier fibresUsedPreferred for fine-denier fibres in the described process
High-denier fibresRecommended for fibres above 8–10 denierSolvent evaporation creates processing difficulties for high-denier fibres
Equipment requirementsCoagulation and washing systemsHeated spinning chambers, gas circulation and solvent recovery

3.1 Fibre Characteristics Obtained by Wet and Dry Spinning

The reported comparison of acrylic fibres spun from DMF solution indicates:

A. Dry-spun acrylic fibres:

  • Higher bulkiness.
  • Better recovery from deformation.
  • Excellent handle.
  • More regular and compact structure.

B. Wet-spun acrylic fibres:

  • Softer handle.
  • Fleecy character, particularly in fine-denier fibres.
  • Higher dye pick-up compared with dry-spun fibres in the described comparison.

4. Dry-Jet Wet Spinning of Acrylic Fibres

Dry-jet wet spinning combines features of dry spinning and wet spinning.

In this method, the polymer solution is first extruded through a spinneret into a short air gap. The filaments then enter a coagulation bath.

The air gap between the spinneret and coagulation bath is reported as 3–5 mm in the described process.

4.1 Process Flowchart

Spinning dope
↓
Extrusion through spinneret
↓
Passage through air gap
↓
Entry into coagulation bath
↓
Filament coagulation
↓
Washing
↓
Drawing
↓
Further processing

4.2 Advantages

  • High-speed fibre formation is possible.
  • Higher dope concentration can be used.
  • High jet stretch can be achieved.
  • Coagulation conditions can be adjusted to control fibre structure.
  • Fine filaments below 1.0 dtex can be produced.

This process helps reduce the formation of large internal voids that can affect the transparency and fibrillation behaviour of wet-spun acrylic fibres.

Infographic


Discover more from Online Textile Academy

Subscribe to get the latest posts sent to your email.

Related Articles

Leave a Reply

Your email address will not be published. Required fields are marked *

Back to top button
error: Content is protected !!

Adblock Detected

Please consider supporting us by disabling your ad blocker